Those who attended Tim Barrett's demonstration at the 1981 AIC conference in Philadelphia may wish to add the following new information to the paper samples and data sheets that were handed out:

Paper Case Paper
 

Prototype

Kozo Tissue

pH of cold water extract:    

blank

7.60 7.60

sample

8.60 8.90
Calcium (%) .9 1.8
 
Copper, ppm 7.7 3.4
Iron, ppm 46.4 32.9
Manganese, ppm 3.1 15.5
Sodium, ppm 30.9 16.8
Magnesium, ppm 176.2 1307.1
Potassium, ppm 0.7 2.1
Zinc, ppm 64.3 215.9
Cadmium, ppm 0.3 0.3
Lead, ppm 19.7 10.3
Antimony, ppm less than 2.6 less than 2.6
Chromium, ppm less than 0.8 8.7
Boron, ppm less than 35.8 less than 35.4

All tests were done on ashed samples using a Perkin-Elmer Atomic Absorption Spectrophotometer. The first nine or ten figures are the items considered worthy of attention. With the exception of a higher preferred calcium content in the paper case paper, these figures seem acceptable to the maker. Comments from conservators, however, are welcome.

Timothy Barrett
5947 N. 25th
Kalamazoo, MI 49004

 [Contents]  [Search]  [Abbey]


[Search all CoOL documents]


URL: http://www.cool.conservation-us.org/byorg/abbey/an/an05/an05-6/an05-613.html
Timestamp: Sunday, 03-Mar-2013 21:33:37 PST
Retrieved: Tuesday, 23-Oct-2018 12:23:54 GMT